Under Extrusion in 3D Printing: Why Prints Have Gaps and Thin Walls
Gaps in the walls, see-through tops, corners that snap: the printer laid down less plastic than it should have. Where the gaps are tells you the cause, so look before you change anything.
You pull a print off the plate and it looks starved. The walls have thin stripes you can see light through, the top has gaps between the lines, and a corner snaps off in your fingers. That is under extrusion: the printer laid down less plastic than it was meant to.
It has a short list of causes and most are free to fix. The trick is to look at where the gaps are before touching any settings, because the location tells you the cause. This guide goes through the patterns, the fixes in order from easiest to hardest, and the numbers saved in our own print-ready designs.
What is under extrusion in 3D printing?
Under extrusion means too little plastic comes out of the nozzle, so the printed lines are too thin to touch their neighbors properly. "Extrusion" is just the word for pushing melted filament out.
The printer cannot see this happening. Prusa's guide makes the point that a printer gets no feedback on how much filament really leaves the nozzle. It turns the gears, assumes the plastic came out, and carries on. That is why a starved print can run for hours without an error.
It matters for more than looks. Prusa describes under-extruded objects as fragile and likely to break apart, because each layer has less material holding it to the next. If you sell your prints, this is a defect to catch before anything goes in a bag.
How do you tell if a print is under extruded?
Look at four places: the walls, the top, the inside and the corners. Bambu Lab's wiki sorts the problem into two types, global (lines are sparse all over the model) and localized (lines are sparse in one area). That one distinction rules out half the causes.

| What you see | Most likely cause | First thing to try |
|---|---|---|
| Gaps all over, from the start | Wrong filament profile, partial clog, low flow ratio | Check the profile matches the spool, then push filament through by hand |
| Fine at first, then a starved band, then fine again | Spool snagged, filament tangled, tube kinked | Spin the spool by hand and look for a crossed loop |
| Fine on slow parts, gappy on fast parts | Filament can't melt fast enough | Raise the nozzle about 10 °C or slow the print |
| Thin only at corners and where the speed changes | Pressure setting is off | Run flow dynamics calibration |
| Only the first layer is thin or see-through | Nozzle too close to the plate | Redo the first layer calibration |
| Starts fine, slowly gets worse, then nothing comes out | Clog building up, or heat softening the filament too early | Clean the nozzle and check the hotend fan |
One check that saves time: run your finger and your eye along the wall at a fixed height. If the fault is at the same height all the way round, something changed at that moment in the print. If it is the same on every layer, it is a setting or a clog.
What causes under extrusion?
Bambu Lab groups the causes into three. In plain English:
- Something is holding the filament back. A spool that won't turn, a tangle, debris or a kink in the plastic feed tube, worn or dirty gears, or a clogged nozzle.
- The printer is asking for more than it can melt. The print is too fast for the temperature, or the filament needs more heat than the profile gives it. A low flow ratio (the setting that scales how much plastic is pushed) belongs here too.
- The timing is off. Pressure inside the nozzle takes a moment to build when the printer speeds up. If the setting that corrects for this is wrong, corners come out thin.
Prusa adds a few more for its own machines that apply widely: a first layer set too close to the plate, the screw that presses the gears on the filament set too loose or too tight, a hotend fan that is blocked or fitted the wrong way round, damp filament, and filament that varies in thickness.
That last one is easy to underestimate. Prusa gives the industry standard as plus or minus 0.05 mm. On 1.75 mm filament, a stretch that is only 1.70 mm thick carries about 5.6% less plastic for the same length, and the printer has no idea.
How do you fix under extrusion, step by step?
Work down this list and stop when the print is solid again. Change one thing at a time, or you won't know what worked.

- Check the spool and the path. The spool should turn freely. Look for crossed loops and for a tight bend or kink in the tube between the spool and the printer.
- Check the profile. In the slicer (the program that turns a model into printer moves), make sure the chosen filament is the one that is loaded. For a brand that isn't listed, Bambu recommends its Generic profile because it prints slower. Prusa also says to start from stock profiles.
- Push filament through by hand. Heat the nozzle and extrude from the printer's screen. A straight, even strand is good. If it curls, sputters or comes out thin, you have a blockage. Our guide to cleaning a nozzle covers the three fixes.
- Dry the filament. Popping sounds and a fuzzy, uneven strand point to damp filament. See how to dry filament.
- Give it more heat or less speed. Bambu suggests about 10 °C more for high-speed printing. Prusa suggests trying 5 to 15 °C either way when a filament has no profile. Stay inside the range printed on the spool. More in our PLA temperature guide.
- Clean the extruder gears. Filament dust packs into the teeth and they lose their grip. Follow your printer maker's steps, with the printer off and cool unless they say otherwise.
- Run the calibrations. Flow dynamics first, then flow rate. On a Bambu printer with Bambu filament, Bambu says to leave the default flow ratio alone, so treat this as a last step.
Safety: a hot nozzle burns on contact, and a blocked one can spit melted plastic when it clears. Keep your face away and wear heat-resistant gloves if you work near it.
Can printing too fast cause under extrusion?
Yes, and on modern fast printers it is worth understanding. Every nozzle can only melt so much plastic each second. That limit is called max volumetric speed, measured in cubic millimeters per second. Bambu's wiki compares it to pouring syrup through a funnel: pour faster than the funnel drains and the flow breaks up.
Bambu's formula is simple: layer height × line width × print speed. A 0.2 mm layer with a 0.45 mm line at 300 mm/s needs 27 mm³ of melted plastic every second. Make the layer thicker and the number climbs again.
The slicer protects you from this. If a line would need more than the filament's limit, it slows that line down by itself. So the danger is not a high speed setting. It is a limit that is too high for the plastic: a raised max volumetric speed, or a fast profile used with a slow-melting filament.
To see the limit in Bambu Studio, click the edit icon next to your filament, stay on the Filament tab and scroll to Max volumetric speed. After slicing, switch the preview colors to Flow to see which parts of the print sit near it. If you are new to the program, start with Bambu Studio for beginners.
What do our own project files use?
We read the saved settings in 656 of our own 3MF project files, across 161 product folders, on 25 November 2026 (including a few older versions we keep on file). A 3MF project stores these settings with the model, which is why you can check them.

- Max volumetric speed: 12 mm³/s in 621 files, 21 in 31, and something else in the last 4.
- Flow ratio: 0.98 in all 646 files set up for PLA, and 0.95 in the 10 set up for PETG. Not one is tuned up to hide a gap.
- Nozzle temperature: 220 °C in all 646 PLA files.
Here is the useful part. In 267 of those files the inner walls are set to 300 mm/s, which by Bambu's formula needs 27 mm³/s, while the filament limit is 12. The slicer holds those walls to about 133 mm/s. The big number in the speed box never happens, and it isn't supposed to.
So if you open one of our files and swap in a filament with a higher limit, the print can speed up a lot without you touching the speed. If gaps appear right after a filament swap, look there first.
What is the difference between under extrusion and over extrusion?
They are opposites. Under extrusion leaves gaps. Over extrusion pushes out too much, so you get blobs, scarred surfaces, ridges on the top and parts that are slightly too big to fit together.
Prusa calls over extrusion a common problem with many filament brands, and notes it shows up most when two flat parts have to be glued. Fits tell the same story: if a lid is suddenly too tight, suspect too much plastic before you suspect the model.
Both are fine-tuned with one setting: flow ratio in Bambu Studio, extrusion multiplier in PrusaSlicer. Prusa says useful values usually fall between 0.9 and 1.1 and adjusts by 1 to 2% at a time. If you need far more than that, the cause is mechanical and the setting is only covering it up.
What looks like under extrusion but isn't?
- Missing lines on a very thin wall. A wall thinner than the line the nozzle draws may be skipped by the slicer. Check the sliced preview: if the gap is there too, it is the model, not the printer.
- Pillowing. A bumpy or holey top over sparse filling. More top layers usually fix it.
- Ripples next to sharp edges. That is ghosting, caused by vibration. The surface is solid, just wavy.
- Wisps between parts. That is stringing, plastic leaking where it shouldn't.
A quick under extrusion checklist
- Where are the gaps: everywhere, one band, or corners?
- Does the spool turn freely?
- Does the chosen filament profile match the spool?
- Does a hand-pushed strand come out straight?
- Is the filament dry?
- Does 10 °C more, or a slower print, fix it?
- Only then: gears, calibration and flow ratio.
A file with known settings makes this easier, because one half of the question is already answered. Our designs come as 3MF projects with the settings saved, plus STL files for any other slicer. If a print from one of them comes out gappy, start with the spool, the filament choice and the nozzle. The license lets you sell the physical prints you make, and the FAQ covers what is in a download.
Designs from this guide
$3.79
3ML-070 · Monitor riser
Monitor Stand
A softly rounded desk riser that lifts your monitor 10 cm, with room to slide a keyboard underneath and a notch at the back for the cables. It goes together by hand: no screws, glue or tools. STL + 3MF · 260 KB View model
$2.49
3ML-098 · Battery organizer
Battery Organizer
A one-piece three-step desk stand for 8 AA, 10 AAA, two 9V batteries and six CR2032 coin cells, with raised labels on every row. STL + 3MF · 1.3 MB View model
$2.49
3ML-083 · Bag clips
Bag Clips
Snack bag clips in three sizes that print in one go with the hinge already inside: fold them shut once and they snap closed. STL + 3MF · 1.2 MB View model
$3.79
3ML-065 · Dice tower
Castle Dice Tower
A stone castle keep for game night: drop your dice in the top, they tumble down hidden ramps and roll out of the arched doorway into a walled courtyard. STL + 3MF · 375 KB View model
$3.79
3ML-147 · Fidget
Heart Gear Fidget
A palm-sized heart with three gears inside. Push any gear with your thumb and all three turn together. It prints flat in one piece with the gears already in place. STL + 3MF · 1.8 MB View modelQuestions
What is under extrusion in 3D printing?
Under extrusion is when less plastic comes out of the nozzle than the printer expects. The lines are too thin to join properly, so the print shows gaps, thin walls and weak layers. The printer cannot detect it, so it keeps going.
What causes under extrusion?
The most common causes are a spool that does not turn freely, a kinked feed tube, a partly clogged nozzle, dirty extruder gears, the wrong filament profile, damp filament, and printing faster than the filament can melt.
How do I fix under extrusion?
Check that the spool turns and the profile matches the filament. Heat the nozzle and push filament through: if the strand is not straight, clean the nozzle. Then dry the filament, try about 10 °C more or a slower print, clean the gears, and calibrate last.
Why is my print under extruding only in one band?
Something interrupted the filament at that height and then let go. A tangled or snagged spool is the usual reason. Bambu Lab calls this localized under-extrusion.
Why are only the corners under extruded?
Pressure in the nozzle lags when the printer changes speed, and corners are where it changes most. Bambu Lab says a wrong pressure advance value causes this and that flow dynamics calibration fixes it.
Can a low temperature cause under extrusion?
Yes. If the nozzle is too cool for the speed, the plastic does not melt fast enough to keep up. Bambu Lab suggests about 10 °C more for high-speed printing. Stay inside the range printed on the spool.
Should I increase the flow ratio to fix under extrusion?
Only as a last step, and only if gaps are visible over the whole print. Bambu Lab advises leaving the default alone with its own filament. Prusa changes it by 1 to 2% at a time. If you need much more, look for a clog or a feeding problem.
What is the difference between under extrusion and over extrusion?
Under extrusion puts down too little plastic and leaves gaps. Over extrusion puts down too much and leaves blobs, rough tops and parts that are too tight to fit. Both can be fine-tuned with the flow ratio once the hardware is ruled out.
Sources
Filed under Printing and slicing